Several techniques are used commonly to reduce profile distortion when air bending with a roll former. These include small-radius forming, false bending, vertical side rolls, and angle side rolls.
When a bend is formed with the air bending process (air bend), the interior of the bending corner can't be reached by either the top roll or the bottom roll, making it difficult to control the part's profile and dimensions. Figure 1 illustrates a typical air bend. The theoretical formed profile is the desired profile. The actual formed profile is the finished part, which was distorted because the top roll couldn't reach the interior corner to hold it in position. The bottom roll flange lifted the section and distorted the profile. Several techniques can reduce such distortion in parts formed by air bending.
The Small-radius Forming Technique
Figure 1
Scoring, grooving, beading, perforating, and interruptive slitting are techniques that can reduce distortion in air bending.
Forming a radius smaller than the metal thickness is a suitable technique for the air bend in Figure 1. Scoring, grooving, beading, perforating, or interruptive slitting weakens the bending track. Scoring is the most commonly used technique. The score depth should not be deeper than one-third the metal thickness in cold roll forming applications. If the score is deeper than one-third the metal thickness, the metal may break at the scored track. In hot roll forming, a grooving track is easy to form and prevents corner cracking.
The beading technique is suitable for thin metal applications. Beading doesn't break the protective coating and doesn't reduce the thickness at the bent section.
A rotary punch performs perforating or interruptive slitting.
The False-bend Technique
Figure 2
Two examples of the false-bend technique show how the bottom section is curved to allow the top roll to make the 90-degree angle at the left side of the part.
The false-bend technique exposes the blind bend (the air bend) to the top roll or bottom roll by curving a straight section (see Figure 2). After the section is curved, the top roll can physically reach the interior bend and form it to 90 degrees precisely. The station after the false-bend station flattens the curve. Usually the false-bend design needs an additional station.
The Vertical Side Roll Technique
Figure 3
A single vertical side roll (A) is better than using conventional rolls. Two vertical side rolls (B and C) provide more precision than a single side roll does.
The vertical side roll located at the outside of the bend is the outer side roll. The forming force from the outer side roll has the same direction as the bending action. It forms a better-quality bend than the conventional rolls in Figure 1. The vertical side roll located at the inside of the bend is the inner side roll. The function of the inner side roll is forming the desired radius at the bend.
The single roll design in Figure 3A cannot control the radius dimension because tooling cannot reach the inner corner. The double side roll design in Figure 3B forms the profile and the dimension more accurately than the roll design in 3A.
The side rolls, which are mounted in the same central line plane as the conventional rolls, are called stationary side rolls, as shown in Figure 3A and Figure 3B. The stationary side rolls and conventional rolls form a rotational extrusion head that squeezes the formed section from all directions: up, down, left, and right. This extrusion process provides strict control over the profile and dimension.
Single side rolls and double side rolls can be mounted before the conventional roll station (see Figure 3C). This arrangement allows more space for large side rolls.
The Angle Side Roll Technique
Figure 4
Angle side rolls can reach the inside corner (A) and the outside corner (B-D) for precise bending.
The double angle side rolls can be mounted before the conventional roll station, as shown in Figure 4D. This is similar to Figure 3C in that it provides more space for large side rolls.
Stationary Mandrel
Figure 5
A roller mandrel is mounted to the roll stand. It is inset into a conventional roll to form an air bend.
Hanhui Li is senior engineer with Worthington Armstrong Venture (WAVE), 9 Old Lincoln Highway, Suite 200, Malvern, PA 19355, 610-722-1232, hanhui_li@armstrong.com.
Reference
George T. Halmos, Roll Forming Handbook (Toronto: Taylor & Francis Group, 2006).
Senior Engineer,
Worthington Armstrong Venture
Hanhui Li is senior engineer with Worthington Armstrong Venture (WAVE), 9 Old Lincoln Highway, Suite 200, Malvern, PA 19355, 610-722-1232. worthingtonindustries.com
hanhui_li@armstrong.com
TAGS: air bending, profiles, roll forming, tooling


Articles