Part II: Forming stainless steel double sinks
November 7, 2006
In deep drawing of complex, asymmetrical parts such as stainless steel kitchen sinks, blank holder force (BHF) needs to be controlled locally to regulate the flow of the sheet metal. An MPC blank holder system allows this control by placing individually programmable cushion pins around the blank perimeter, with an appropriate BHF selected at each pin location.
Editor's Note: This article is Part III of a three-part series on multipoint-control (MPC) die cushion systems. Part I, which appeared in the September issue, discussed novel press and design concepts using MPC systems. Part II, which appeared in the October issue, covered MPC systems applied to the forming of stainless steel double sinks. Part III discusses prediction of blank holder force.
This column was prepared by Ajay Yadav and Hariharasudhan Palaniswamy of the Center for Precision Forming (CPF) (formerly Engineering Research Center for Net Shape Manufacturing), The Ohio State University, Taylan Altan, professor and director.
Modern presses that are equipped with multipoint-control (MPC) die cushion systems allow the blank holder force (BHF) to vary during the press stroke. This capability is currently underused because BHF prediction in each cushion pin is time-consuming and expensive.
With constant BHF, conventional steel sheets can be formed with few tryouts. However, with the increasing use of lightweight materials and high-strength steels with low formability, there is a need for precise, localized control of metal flow using MPC systems. For increasingly complex parts, MPC can expand the process window.
Four possible ways to apply BHF during forming with an MPC unit are:

Figure 1
Methodology to estimate BHF in MPC die cushion systems involves numerical optimization techniques coupled with FE simulation. Tool geometry, sheet material properties, and process conditions are necessary inputs for accurate simulation.
The CPF has developed a methodology to predict BHF in each MPC cushion pin for all four possible configurations
(see Figure 1). The methodology combines numerical optimization techniques with finite element (FE) simulation to estimate the BHF needed to form a wrinkle-free part with minimal thinning.
This estimated optimal BHF profile determined from FE simulations serves as an excellent starting point for die tryouts, which can considerably reduce die development time.
The methodology has been used to predict BHF for MPC systems with hydraulic or nitrogen cylinder cushions, as well as for single-point cushion systems.
An automotive liftgate inner panel was successfully formed with minor wrinkles using the developed methodology. It should be noted that an aluminum-alloy liftgate inner panel initially could not be formed using a conventional single-point system despite repeated tryouts. This demonstrates how an MPC system can enhance the conventional stamping process to form autobody panels from lightweight materials.

Figure 2
Estimated BHF is constant over the punch stroke to form this 1mm-thick A6111-T4 aluminum alloy.
Using this methodology, the CPF estimated BHF for different sheet materials and thicknesses (seeFigure 2). Liftgate panels in Figure 3awere formed successfully from three different materials and sheet thicknesses in the same die, without any physical modifications. Figure 3bshows a sample BHF profile (with BHF varying in location over blank holder surface and changing with punch stroke) used to successfully form a 1-mm-thick A6111-T4 aluminum-alloy sheet.

Figure 3a
With MPC a liftgate panel was formed successfully from three different materials and sheet thicknesses in the same die, without any physical modifications.
BHF profiles were similarly estimated for bake-hardened steel (BH210, t = 0.8 mm) and high-strength steel (DP500, t = 0.8 mm). In both cases, the use of an MPC system resulted in a robust stamping process that can account for variations in incoming sheet material and thickness.1
MPC technology also can be used in sheet hydroforming. Estimated BHF profiles for sheet hydroformed parts using MPC systems were discussed in the April 2006 issue, p. 26.
Taylan Altan is a professor and director of the Center for Precision Forming. The CPF conducts research and development; educates students; and organizes workshops, tutorials, and conferences for the industry in stamping, tube hydroforming, forging, and machining.