Part II of this series presented a basic overview of metal forming operations, such as bending, flanging, drawing, ironing, coining, curling, hemming, and embossing. This and future installments discuss these operations in more detail. We will look at factors controlling the success of each operation, as well as tooling design guidelines. Let's begin with metal bending, a process often perceived as the simplest.

Bending

Bending can be defined simply as a forming operation in which the metal is deformed along a straight axis. Both compression and tension occur when bending sheet metal. The inside radius of the bent metal is in compression, or being squeezed together. The outside bend radius is in tension, or being stretched.

Because of the metal's elastic properties, it wants to decompress on the inside radius and return to its flat shape on the outside radius (Figure 1), which causes springback. Also know as elastic recovery, springback is present in all metal bending operations.

Springback diagram

Figure 1

For a 90-degree bend angle, the metal must be bent to an acute angle (less than 90 degrees) and allowed to spring back to its finished position, a difficult task given the fact that a press ram typically travels vertically only. In addition, because of natural mechanical variability in the material from coil to coil and from the beginning of the coil to its end, attempting to achieve a consistent, precision angularity in a bending operation can be very difficult.

If ultraprecision bend angles are required, one of the best things you can do to achieve them is to design the tool so that it can be adjusted quickly, safely, and effectively to compensate for incoming variables.; Changing the product design also can help reduce springback and inconsistency problems. Incorporating darts, ribs, or gussets into the part design will enhance stiffness and reduce the amount of springback (Figure 2).

Stiffening Ribs images

Figure 2
Photos courtesy of Batesville Tool and Die Company.

Bending Methods

Several basic types of bending methods can be incorporated into a stamping operation—wipe bending, V bending, and rotary bending. All three are popular, and each has its advantages and disadvantages.

Wipe Bending—One of the most common methods used, but not always the most effective, is simple wipe bending. Unfortunately, this method does not allow for much overbending other than the very slight acute angle that can be achieved by wiping the side extremely tight (Figure 3). Even though wipe bending effectively creates a bend, controlling the bend angle is very difficult. This method is not well-suited to bending high-strength metals or for parts requiring precision bend angle tolerances. Wipe bending can be improved by capturing the outside profile of the radius with the forming die section.

Wipe Bending diagram

Figure 3
Simple wipe bending method

Figure 4shows a coin relief method. This process allows the outside radius to be coined, or squeezed, near the lower tangent point, which causes under- or over -bending to take place. The coin relief method works best when the metal is bent over a radius that is equal to or less than one metal thickness, and the metal is not ultrahigh-strength. One advantage to this method is that by vertically shimming the forming section up and down, the gap, as well as the amount of coining, can be adjusted. This allows for easy adjustments to be made for variability in the metal's thickness and mechanical properties.

Coin relief bending method

Figure 4
Coin relief bending method

Figure 5shows a pivot-style bending method, which incorporates both wipe bending and cam motion. This design works well both to create the bend and to adjust the amount of overbend. Overbend is created by adjusting the lower driver block vertically up and down.

Pivot style bending diagram

Figure 5
Pivot style bending design

V Bending—A very good method for obtaining a given bend angle, V bending is undoubtedly the most common method used with press brake bending. An acute angle ground on both the punch and die can provide adequate overbending of the metal. Also, the bending amount can be altered by adjusting the amount of coining the metal undergoes at the bottom of the press stroke (Figure 6).

V bending method diagram

Figure 6
V bending method

One disadvantage to V bending is that it often requires the part to be rotated in such a manner that sometimes is difficult to incorporate in a progressive die. An advantage is that it often requires less force to create the bend compared with conventional wipe bending.