- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
R&D Update: Examining edge cracking in hole flanging of AHSS, Part II
Part II: Modeling of blanking
- October 4, 2017
- Article
- Bending and Forming
A number of studies have shown that the edge quality of the punched hole has a significant influence on hole stretchability. For example, holes made by wire EDM have a better stretchability than drilled or sheared holes. Another study showed that blanking, which is the most practical method of producing holes or cutouts, generates a shear-affected zone (SAZ) and a burr, and if these are removed, hole stretchability increases.
It is useful to characterize the sheared edge quality, produced by blanking, through experiments and computer simulations.
Ultimately, the aim is to be able to quantify how deep a flange can be achieved, or how much a hole can be expanded, for a given blanked or sheared edge quality.
The sheared edge (see Figure 1 consists of:
- The shear zone, which is smooth and shiny and created by shearing the material.
- The fracture zone, where fracture causes the part to separate from the blank sheet.
- The depth of crack penetration, which is a deviation from a straight part edge.
- The rollover zone, where the edge of the sheet surface is bent by plastic deformation.
In addition to the geometric features, the sheared edge quality also includes the SAZ, which extends from the sheared surface into the adjacent material. The SAZ is the volume of metal that has been subjected to a very high plastic deformation and high temperature during shearing. Thus, the sheared edge quality (geometry and SAZ) is affected by the punch-die clearance, material properties, material thickness, cutting speed, and tool wear.
Effects of Punch-Die Clearance on Sheared Edge Geometry
Blanking experiments conducted at the CPF with AISI 1050 sheet are shown schematically in Figure 2 . Different die diameters were used for setting different punch-die clearances, such as 5 percent, 10 percent, and 15 percent of the sheet thickness. The edge of the blanked sheet, obtained from the tests, was sectioned and put under an optical microscope to measure the sheared edge geometries.
Experimental results are summarized in Figure 3 . As the punch-die clearance increases within the range investigates:
- The rollover zone (plastic deformation of the sheet before separation) increases.
- The shear zone decreases.
- The fracture zone increases slightly.
- The burr height remains approximately uncharged.
FE Simulation of Blanking
Finite element (FE) simulations of blanking were conducted to predict the shear edge geometries and the SAZ more accurately. The initial setup of the FE model is illustrated in Figure 4 . Calculated steps of blanking are shown in Figure 5 , which illustrates that strains in the shearing zone kept increasing until cracks initiated, causing fracture. FE modeling of blanking is improved by including a fracture criterion that indicates when the cracks initiates in the simulations. Figure 6 shows the sheared edge obtained from blanking tests and simulation at a punch-die clearance of 15 percent.
The effect of temperature needs to be considered in the FE model, since a very large plastic deformation and temperature increase occurs in a localized deformation zone. Simulation shows that local temperature increases up to 440 degrees C can occur in blanking of AISI 1050 sheet (see Figure 6b). This temperature could be higher in blanking AHSS because these steels have a higher strength and lower thermal conductivity than AISI 1050.
subscribe now
The Fabricator is North America's leading magazine for the metal forming and fabricating industry. The magazine delivers the news, technical articles, and case histories that enable fabricators to do their jobs more efficiently. The Fabricator has served the industry since 1970.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 04/16/2024
- Running Time:
- 63:29
In this episode of The Fabricator Podcast, Caleb Chamberlain, co-founder and CEO of OSH Cut, discusses his company’s...
- Trending Articles
Tips for creating sheet metal tubes with perforations
Supporting the metal fabricating industry through FMA
JM Steel triples capacity for solar energy projects at Pennsylvania facility
Fabricating favorite childhood memories
Omco Solar opens second Alabama manufacturing facility
- Industry Events
16th Annual Safety Conference
- April 30 - May 1, 2024
- Elgin,
Pipe and Tube Conference
- May 21 - 22, 2024
- Omaha, NE
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI