Manager of Specialty Gas Products
- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Oxyfuel brazing primer
Info, tips, and tricks for an optimal process
- By David Gailey and Robert Henson
- March 19, 2014
- Article
- Assembly and Joining
Oxyfuel brazing is a simple yet effective method for joining metal that produces sound, leakproof connections. In brazing, an oxyfuel torch is used to heat the base metal to the correct temperature—above the melting point of the filler metal but below the base metal’s melting point. Capillary action then draws the melted filler metal between the two closely fitted surfaces to form an ideal seal.
When oxyfuel brazing is chosen over welding for metal joining it is because the process is simple to perform, does not melt or otherwise distort the base metals, and allows for high tolerance control. Another reason that many people opt for brazing is the ability to produce joints without the need for secondary finishing and to allow joining of dissimilar materials.
Manual oxyfuel brazing of copper is common throughout industry, especially in air-conditioning and refrigeration applications. Here’s a primer on the popular process.
Differentiating Between Soldering and Brazing
One of the main differences between brazing and soldering is working temperature. Soldering takes place below 840 degrees F and uses tin as the primary alloying element. Braze alloys are copper-based and tend to melt at higher temperatures—above 1,190 degrees F for copper joining. Both soldering and brazing provide seals via the previously mentioned capillary action, where the melted filler flows into the space between a tube and fitting, known as the capillary space, and adheres to the tube and fitting surfaces. Brazing delivers greater fatigue resistance and developed joint strength than soldering.
Brazing is used in both repair and high-volume manufacturing. While repair entails manual brazing, manufacturing uses manual and automated brazing in operations large and small. For example, residential air conditioners, with thousands sold of each model, requires automated flame brazing of copper U-bends in an assembly line production method. Commercial airconditioning units, on the other hand, are often batch-produced in smaller volumes. For these assemblies, manual brazing provides the necessary versatility and efficiency.
Common Brazing Alloys for Copper
Copper-to-copper joining primarily employs two families of brazing alloys, designated by the American Welding Society as BCuP and BAg.
BCuP (B = Brazing; Cu = Copper; P = Phosphorus). This is a copper-phosphorous alloy that contains anywhere from 0 to 18 percent silver. Phosphorus serves as a deoxidizer, which eliminates the need for a separate chemical flux. It also lowers the alloy’s melting point. Silver acts as a wetting agent to improve adherence, and its addition also contributes to lowering the alloy’s melting point. This alloy family is the most frequently used for copper brazing (it is not designed to braze steel or other ferrous metals).
BAg (Ag = Silver). This alloy typically contains roughly 20 to 72 percent silver and can be used to braze copper with a flux, but most often is used to braze copper to other metals like brass or steel.
Make Sure Tubes and Fittings Are Square and Clean
Properly prepared base metal is a key factor in successful brazing. Cut the tube or pipe with a tube cutter to exact length and square. If you are using a hacksaw, be sure to use a sawing fixture to achieve a square cut. Also, remove any burrs from the inside and outside diameters and make sure that the tube is not out of round (see Figure 1).
The joint surface areas must be clean, so remove oil, grease, or oxide contamination. A stainless steel wire brush, emery cloth, Scotch Brite®, or similar abrasive will work just fine. Use commercial solvents to remove oil and grease and then wipe down the tube and fitting surfaces with a clean, dry cloth.
If one metal is brass or bronze, you must use a flux. Apply a thin layer of flux with a brush and assemble the tubes and fittings. Maintain support so that the workpiece remains aligned properly, at least until a few seconds after brazing.
HVAC, medical gas, and other critical applications require an inert gas—typically nitrogen—to purge the inside of the tube during brazing. The nitrogen displaces the oxygen and prevents oxide scale from forming inside the tube.
Remember to Add Heat Uniformly
Most oxyfuel brazing processes call for a slightly carburizing or neutral flame. A neutral flame has a bright-blue, well-defined inner cone, while a carburizing flame has a less defined, or feathered, inner cone. Carburizing flames, if correctly set, remove surface oxides from the copper and help improve the appearance. Avoid an oxidizing flame. Remember, the goal is cleaning and fluxing to remove metal oxide and protect the part during heating. The oxidizing flame promotes oxidation, which will inhibit braze-alloy flow.
To start, apply the flame at a point just adjacent to the fitting and heat the tube first (see Figure 2).
Then work the flame alternately around the tube and fitting (see Figure 3) using short motions until both reach brazing temperature.
Keep in mind that flux is a good temperature indicator. Continue heating until the flux completes a bubbling phase and becomes quiet, fluid, and transparent—like water. This is a visual cue that parts are close to brazing temperature. To maintain uniform heat in the tube and fitting, sweep the flame back and forth along the axis of the tube, joint, and fitting.
Next up is adding the brazing alloy.
Apply Brazing Alloy, Ensure Joint Fill
The brazing alloy, in wire or rod form, should be fed into the joint between the tube and fitting (see Figure 4).
Again, do this only after the base metals have been heated to brazing temperature. Direct the flame to the tip of the brazing alloy to begin the melting process and continue sweeping the flame back and forth over the tube and fitting as the alloy is drawn into the joint.
If the brazing alloy must move vertically up from the tube into the joint, apply heat to the tube first, then the fitting, ultimately bringing both pieces to temperature evenly. Keep the flame directed toward the fitting, because if the tube overheats, the brazing alloy may run down the tube rather than into the joint.
The alloy will fill all joint areas, assuming that you have prepared the joint properly, reached brazing temperature, and selected the appropriate brazing alloy. There’s no need to feed more brazing alloy once the joint is filled; doing so offers no added benefits and only wastes the alloy.
As soon as the brazing alloy has set, use a wet swab or brush on the joint end to remove any flux residue. An emery cloth or a wire brush can be used if necessary. For proper inspection and pressure testing, be sure to remove all residue. If the process is performed properly, brazing will deliver a fully sealed joint.
Avoid Typical Brazing Pitfalls
As with any joining process, there are pitfalls. Here are some common problems that you may encounter as well as some advice on how to fix them.
Pitfall No. 1: The outside of the joint is hot, but the inside is not hot enough. Remember to heat the tube first, which will conduct heat into the fitting to raise the inside temperature.
Pitfall No. 2: The flux has broken down due to excessive heat. Flux can become saturated with oxides if it is overheated, preventing flow of the brazing alloy. A softer flame or a heavier coating of flux will help.
Pitfall No. 3: The brazing alloy balls up instead of running into the joint. Either the base metals have not reached brazing temperature, and the alloy has been melted by the torch flame, or the joint has overheated, resulting in flux that no longer is active. Review the heating procedure. Another possibility is that the base metals are not properly cleaned.
Pitfall No. 4: The brazing alloy flows away from, instead of into, the joint. The fitting may not have reached the proper brazing temperature. Direct the flame toward the fitting.
Pitfall No. 5: The brazing alloy cracks after it solidifies. With copper connections especially, a likely cause is insufficient braze penetration into the joint. This may cause the brazing alloy to crack under stress or vibration. Be sure to hold to recommended clearance and review your brazing technique.
This also can occur if you are brazing dissimilar base metals, especially if they are quenched too quickly. Let the joint cool for a longer period before you wash off the flux residue.
About the Authors
David Gailey
2345 Murphy Blvd.
Gainesville, GA 30501
678-928-3801
Robert Henson
Technical Director
4501 Quality Place
Mason, OH 45040
513-754-2000
About the Publication
subscribe now
The Welder, formerly known as Practical Welding Today, is a showcase of the real people who make the products we use and work with every day. This magazine has served the welding community in North America well for more than 20 years.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 04/30/2024
- Running Time:
- 53:00
Seth Feldman of Iowa-based Wertzbaugher Services joins The Fabricator Podcast to offer his take as a Gen Zer...
- Trending Articles
Aluminum MIG wires offer smooth feeding, reduced tangling
The role of flux in submerged arc welding performance
Three ESAB welding machines win Red Dot Awards for product design
Power source added to cobot welding system for simplified automation
Torch made for welding thin, conductive sheet metal
- Industry Events
Pipe and Tube Conference
- May 21 - 22, 2024
- Omaha, NE
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI
Precision Press Brake Certificate Course
- July 31 - August 1, 2024
- Elgin,