- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Ask the Stamping Expert: How can I prevent slivers in blanking operations?
- By Thomas Vacca
- May 27, 2016
- Article
- Bending and Forming
Q: We are making shallow drawn cuts from 0.007-inch-thick aluminum base material with a thin polymer coating. The cups are assorted sizes from 0.375 to 0.75 in. and equal depths. We pierce the blank and use a Ballantine to carry it in the strip web through the draw operations, and finally we pinch-trim it through the die. Our problem is that slivers generated in blanking accumulate in the tool and mark the drawn cups. What can we do?
A: For cutting aluminum in Ballantining for drawing in a progressive die, C2 carbide grades are preferable. They are very hard and keep the sharp edge very well.
For punching, the carbide grade depends on the cross section of the punch. The thicker the cross section, the harder the carbide should be. To mitigate breakage of whole punches, sometimes a hybrid punch with a small carbide tip silver-brazed in place is preferable.
When using carbide for machining processes, the tip must be radiused and mirror-polished. For punching in a progressive die, the face and the walls of the punch also must be mirror-polished; otherwise, as speed increases, microwelds of aluminum will adhere to the walls of the punch in areas of microscopic surface imperfections, creating slivers as they pass through the strip.
If you’re cutting punches with wire EDM, use caution. The process pulls out the cobalt binder used in the manufacture of carbide, causing a work-affected zone on the surface. While multiple skim cuts can nearly eliminate the work-affected zone, grinding still yields the best results for very fine and critical applications.
If the grinding lines are parallel to the front of the punch, the punch will act as a fine file and generate slivers. Grind all punches in the same axis as the punching motion whenever possible.
Sometimes slivers are a function of the clearance between the punch and die. Extra clearance will result in less friction between the blank and the walls of the die as you push the blank back up into the strip.
Another way to avoid small slivers is to use a negative angle in all punches. The negative angle is measured in ten-thousandths of an inch. On a 2-in.-long punch, the punch size at the back end may be smaller by 0.0006 to 0.0008 in.; the cutting end of the punch would be larger by the same amount.
To lap the sides of a round punch without getting a barrel-like shape, try a copper disk 0.25 to 0.375 in. thick after grinding the punch sides to 0.02-degree negative taper.
When polishing, you might assume that the sides are parallel, but it’s best to inspect them under a microscope and measure them with a fine precision micrometer. Any punch with a smaller front than back might create small filings.
For pesky slivers caused by the slug breaking through the material, you could inject very light lubricant into the bottom side of the strip and on top of the die to disperse the slivers and prevent marking of the manufactured parts. The press will need to be modified to reclaim the oil by passing it through a filtration system before it can be recirculated.
Many times when a punch is reworked, not all of the worn-out surface is removed. When servicing your punches, inspect the edge under a stereomicroscope at 200-to-1 minimum to see the remaining microscopic negative cutting edge. This will show you how much material to remove to prevent chip generation.
The author gratefully acknowledges the advice of Wilson J. Cubides in the preparation of this article. Cubides, a graduate of the National University of Colombia with a degree in mechanical engineering, has more than 40 years of experience in the stamping, coining, cold heading, and drawing industries. He can be reached at williecad@aol.com.About the Author
Thomas Vacca
Micro Co.
Has a shop floor stamping or tool and die question stumped you? If so, send your questions to kateb@thefabricator.com to be answered by Thomas Vacca, director of engineering at Micro Co.
subscribe now
The Fabricator is North America's leading magazine for the metal forming and fabricating industry. The magazine delivers the news, technical articles, and case histories that enable fabricators to do their jobs more efficiently. The Fabricator has served the industry since 1970.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 04/16/2024
- Running Time:
- 63:29
In this episode of The Fabricator Podcast, Caleb Chamberlain, co-founder and CEO of OSH Cut, discusses his company’s...
- Trending Articles
Tips for creating sheet metal tubes with perforations
Supporting the metal fabricating industry through FMA
JM Steel triples capacity for solar energy projects at Pennsylvania facility
Fabricating favorite childhood memories
Omco Solar opens second Alabama manufacturing facility
- Industry Events
16th Annual Safety Conference
- April 30 - May 1, 2024
- Elgin,
Pipe and Tube Conference
- May 21 - 22, 2024
- Omaha, NE
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI