- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Ask the Stamping Expert: How do we prevent buckling in thin material during strip feeding?
- By Thomas Vacca
- July 6, 2016
- Article
- Bending and Forming
A: This is a very common problem with a couple of very achievable solutions, each with its own benefits and drawbacks:
- Mount a pull feed on the exit end.
- Use a push feed.
Pull feeding is more expensive, because you will need to invest in a feed—most likely a servo-driven hitch feed. You also will have the expense of mounting the feed on the press and installing the electronics required for the feed to communicate with the press.
In addition, you will have to design and build the brackets and stamped raw material webbing guides between the die and the feed, and then determine what to do with the webbing. If volume makes it cost-effective, you could invest in a scrap chopper. We have done this by purchasing an off-the-shelf scrap chopper and building a frame. The frame accommodates the chopper sitting on top of a 55-gal. steel drum. When the drum is full, we lift it off and replace it with an empty drum.
I estimate you will spend about $30,000 on a pull feed, $15,000 on electronics (you will need a resolver), $25,000 on a PLC interface, and $10,000 on engineering and fabrication of miscellaneous brackets and liners. If you add the scrap chopper, you have a $100,000 project. It will work very well, and if you can justify the cost, this is the way to go. Pulling the material is much easier than pushing it, without a doubt.
The other option is push feeding, which is the type of feed you have. This feed uses partial roll segments rather than a full-diameter roller. The upper and lower roller segments basically rock back and forth to feed the material.
The space between the feed rollers and the die entrance must be filled with a liner to contain the material—basically two plates of hardened steel with a groove ground between them to accept the raw material. The groove should be 0.005 to 0.010 in. deeper than the material thickness. In this case, start with 0.010 to 0.015 in. and grind deeper if needed. This is critical to prevent the material from buckling.
Next, test the liner by hand with a piece of cut strip stock. This will help you develop a nice slip fit of the strip in the liner, but not so sloppy as to allow the material to ripple within the liner. This can cause slight variations in feed length in the tool as material accumulates in the liner and then springs forward.
There are three keys to making this work:
- Bring the top and bottom liner plates to a knife edge so they can be positioned as close as possible to the feed rollers and end as close as possible to the tool entrance.
- Scallop both plates to relieve the surface area. We would grind a series of 1/16-in.-wide grooves, 0.010 in. deep at 0.072-in. centers, along the entire length of the material liner grooves. This leaves a series of 0.010-in.-wide bearing surfaces. Be sure to polish them to prevent scratching of the raw material.
- Drill and tap a hole to accept an airline fitting in the center of the bottom liner. Feed in 5- to 10-PSI compressed air to float the coil stock as it passes through the liner. Try it on the bench while adjusting the air to feel for the optimal pressure that yields the best results. You will be amazed! The strip will virtually float and move through the liner with very little resistance. Cut out a small window across the liner wider than the raw material, about 3/16 in. wide, to allow mounting of a mist spray lubrication unit to oil the top and bottom of the stock.
About the Author
Thomas Vacca
Micro Co.
Has a shop floor stamping or tool and die question stumped you? If so, send your questions to kateb@thefabricator.com to be answered by Thomas Vacca, director of engineering at Micro Co.
subscribe now
The Fabricator is North America's leading magazine for the metal forming and fabricating industry. The magazine delivers the news, technical articles, and case histories that enable fabricators to do their jobs more efficiently. The Fabricator has served the industry since 1970.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 04/16/2024
- Running Time:
- 63:29
In this episode of The Fabricator Podcast, Caleb Chamberlain, co-founder and CEO of OSH Cut, discusses his company’s...
- Trending Articles
Tips for creating sheet metal tubes with perforations
Supporting the metal fabricating industry through FMA
JM Steel triples capacity for solar energy projects at Pennsylvania facility
Fabricating favorite childhood memories
Omco Solar opens second Alabama manufacturing facility
- Industry Events
16th Annual Safety Conference
- April 30 - May 1, 2024
- Elgin,
Pipe and Tube Conference
- May 21 - 22, 2024
- Omaha, NE
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI