- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Minimizing start stop welding defects
- By Paul Cameron
- Updated February 8, 2024
- May 5, 2014
- Article
- Arc Welding
Q: I am having trouble making welds that are all the same length when using GMAW. How can I create tie-ins that are all in line with each other and spaced out as they should be?
Allen T.
A: It is understood throughout the industry that most weld defects are attributed to weld stops and starts. We automate (or change from manual to semiautomatic) to improve cycle time and quality. Most of that quality improvement comes from eliminating starts and stops. Welding starts can lead to overlap, incomplete fusion, and slag inclusion, while stops typically lead to cracks and undercut.
Some of these discontinuities may be considered acceptable, but stacking them on top of one another in a multipass weld is just flirting with disaster.
Stops and starts are a necessary evil in welding. We can minimize their negative effects, however, through techniques during manual welding and through weld data settings for semiautomatic and automated welding.
Optimizing Your Weld Settings
In GMAW those weld settings that can be added to many wire feeders include:
- A burnback that keeps the wire stickout as short as possible will help with your next arc start.
- A three-second postflow protects the wire and keeps it clean.
- A preflow (0.2 second) ensures the shielding gas covers the area before an arc is struck.
- A slow run-in speed of -100 to -200 will reduce the “snap” that often occurs when initially striking an arc.
- Increasing the start by 1 or 2 volts will also reduce the snap.
Work on Your Welding Technique
As for your welding technique:
- When striking an arc, begin ahead of the desired start point (1½ times the weld size). After you strike the arc, back up quickly to the desired start point then begin your weld. This will almost eliminate any overlap (cold lap) that is common with weld starts.
- When extinguishing the arc, weld to the desired stop point then back up (1½ times the weld size). This will fill the weld crater, slow the cooling rate, fill the undercut, and reduce the chances of a crater crack.
You could probably search the Internet for an article on weld stops and starts and get plenty of horror stories. In that same search you will find oodles of “pixie dust” salesmen with quick-fix products or equipment that claim to take all those troubles away.
Stick with common sense. Equip your feeders with the settings that help improve weld starts and stops, and be sure to use good welding techniques.
About the Author
Paul Cameron
Braun Intertec
4210 Highway 14 East
Rochester, MN 55904
About the Publication
subscribe now
The Welder, formerly known as Practical Welding Today, is a showcase of the real people who make the products we use and work with every day. This magazine has served the welding community in North America well for more than 20 years.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 04/30/2024
- Running Time:
- 53:00
Seth Feldman of Iowa-based Wertzbaugher Services joins The Fabricator Podcast to offer his take as a Gen Zer...
- Trending Articles
Aluminum MIG wires offer smooth feeding, reduced tangling
The role of flux in submerged arc welding performance
Three ESAB welding machines win Red Dot Awards for product design
Power source added to cobot welding system for simplified automation
Connecticut students compete in Maritime Welding Competition
- Industry Events
Pipe and Tube Conference
- May 21 - 22, 2024
- Omaha, NE
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI
Precision Press Brake Certificate Course
- July 31 - August 1, 2024
- Elgin,