President
- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Aluminum Workshop: Defining porosity in aluminum welds
- By Frank Armao
- Updated August 8, 2023
- September 28, 2015
- Article
- Aluminum Welding
Q: I’m having quite a bit of trouble with porosity in my aluminum welds lately. Can you tell me the sort of measures I should take to minimize the porosity?
A: Let’s first define the basic cause of weld porosity in aluminum and then go on to summarize the major causes.
All porosity in aluminum welds is caused by hydrogen in the weld. Though solid aluminum has a very low solubility for hydrogen, molten aluminum has a very high solubility for hydrogen. While the weld metal is in the molten state, it absorbs a lot of hydrogen. It will then try to expel the hydrogen as the weld metal solidifies. If the weld is solidifying even moderately quickly, it can’t rid itself of the hydrogen, which stays behind and forms porosity.
So, where exactly does this hydrogen come from? After all, there is only a very small amount of hydrogen in the air. The hydrogen comes from one of two possible sources – either water vapor or hydrocarbon contamination (i.e., oils, greases, lubricants, and solvents). If any of these substances gets into the arc, the heat from the arc breaks them down into hydrogen and other substances. There’s the cause of your porosity.
Minimizing Porosity in Aluminum Welds
Minimizing porosity is mostly about cleanliness and housekeeping. There are actually many possible causes of porosity. Following are the top four culprits and how to prevent them from happening.
- Poor Preweld Cleaning. Be sure to degrease the part before you weld. Wipe down the surface of the material with a clean, lint-free rag saturated with a good degreasing solvent. Acetone and toluene are among the best. Alcohols are not good degreasers and should not be used for preweld cleaning. Following degreasing, the aluminum surface is then deoxidized, usually by using a stainless steel wire brush. Mistakes here are the most common cause of porosity.
- Insufficient Shielding Gas Flow Rate. For gas metal arc welding (GMAW), the flow rate should be at least 35 SCFH, although flow rates up to 60 SCFH can be used, especially with big gas nozzles. Argon/helium gas mixtures require even higher flow rates. For gas tungsten arc welding (GTAW), the flow rate should be at least 25 SCFH.
- Incorrect Nozzle-to-Work Distance. Simply put, this distance should be as small as possible, preferably in the range of ½ to 5/8 in. Longer nozzle-to-work distances can suck in surrounding air and other contaminants.
- Improper Gun Angle. Aluminum welding always requires a leading gun angle. If you try to use a drag angle or even a 90-degree angle, you will get porosity in your welds.
About the Author
Frank Armao
Aluminum Consulting Inc.
440-479-0239
About the Publication
Related Companies
subscribe now
The Welder, formerly known as Practical Welding Today, is a showcase of the real people who make the products we use and work with every day. This magazine has served the welding community in North America well for more than 20 years.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 04/16/2024
- Running Time:
- 63:29
In this episode of The Fabricator Podcast, Caleb Chamberlain, co-founder and CEO of OSH Cut, discusses his company’s...
- Trending Articles
Sheffield Forgemasters makes global leap in welding technology
ESAB unveils Texas facility renovation
Engine-driven welding machines include integrated air compressors
How welders can stay safe during grinding
The impact of sine and square waves in aluminum AC welding, Part I
- Industry Events
16th Annual Safety Conference
- April 30 - May 1, 2024
- Elgin,
Pipe and Tube Conference
- May 21 - 22, 2024
- Omaha, NE
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI